Guide 01 · about 45 minutes
Removing an etch ring from polished marble
A single ring where a glass or a bottle stood takes about forty-five minutes including the test patch, and needs roughly 20 g of compound. The method matters less than knowing when to stop, so that part comes first.
Step zero: prove it is an etch
Two tests, thirty seconds, and they decide whether this page is relevant at all.
- Low light. Hold a torch almost flat to the surface and look along it. An etch appears as a dull shape that vanishes when you look straight down. A stain is visible from every angle.
- Wet it. Wipe the mark with a damp cloth. A stain goes darker and more obvious while wet; an etch looks almost repaired and then returns as the water evaporates.
If both say stain, go to the diagnosis table instead â compound on a stain will polish the discolouration to a high shine and nothing else.
What you need
- LOOP-P2, about 20 g per 30 × 30 cm of damage
- A white polishing pad: by hand for one ring, or on a machine at 150â300 rpm for anything larger
- A spray bottle of clean water, and two clean microfibre cloths
- Nitrile gloves and goggles - the compound is acidic, see safety
- A torch, for judging the result properly rather than hopefully
Method
- Mask anything within 300 mm that is metal, glass or mirrored. Compound hazes glass and dulls chrome, and both are harder to put right than the etch.
- Do a test patch somewhere nobody looks - under a kettle, behind a tap, inside the edge of a cupboard. One 90-second pass. If gloss returns there, continue; if the stone instead looks slightly cloudy, stop and read the last section of this page.
- Clean and dry the area. LOOP-N4 at 1:60, rinsed and dried. Grit under a pad cuts scratches faster than compound removes them.
- Apply about 20 g over the ring and 50 mm beyond it, so the repair has somewhere to blend into.
- Work it for 90 seconds in overlapping circles, light pressure, pad kept damp with the spray bottle. The paste should stay creamy; if it starts to dry, mist it rather than pressing harder.
- Wipe clear and dry, then inspect with the torch at a low angle. Wet stone always looks finished, which is why this step is done dry.
- Repeat at most twice more. Three passes is the limit. If the third changes nothing, the damage is deeper than this product reaches.
- Rinse, dry, wait 24 hours, then re-seal that patch with LOOP-S1 - four minutes of dwell, all excess wiped off. Polishing removed whatever sealer was there, and an unsealed patch on a worktop will stain within the week.
What a good result looks like
The repaired area matches the stone around it from every angle, including the low one. If it is shinier than its surroundings you have polished too long: take one very light pass over a much wider area to feather the difference outwards. That is far easier than trying to dull the patch back down.
| Job | Compound | Time | Realistic outcome |
|---|---|---|---|
| One ring, about 100 cm² | 20 g | 45 min | Invisible in normal light |
| Several rings on a 2 m² worktop | 250â300 g | 3â4 h | Much improved; a faint map may show in raking light |
| A whole etched worktop or vanity | - | - | Hand it to a contractor for honing and polishing as one surface |
Stop and call somebody if
- Your fingernail catches the edge of the mark. That is depth, not dullness, and polishing a hollow makes it a deeper hollow.
- More than about a quarter of the surface is etched. Patch repairs will leave a visible pattern; the whole piece wants doing at once.
- The finish is honed, tumbled or brushed. LOOP-P2 would leave a gloss patch - the compatibility table marks this as never.
The four ways this goes wrong
A coloured pad. Red, green and black pads carry their own abrasive and leave swirl marks that only show up once the gloss returns. White only.
Letting the compound dry. Dried paste has to be softened again before removal, and on soft marble the scrubbing does more harm than the etch did.
Too much machine pressure. A heavy machine held in one spot cuts a shallow dish that catches the light forever. Keep it moving; let the abrasive work rather than your arms.
Skipping the re-seal. This is the one we hear about most, usually a fortnight later, when a coffee cup has left a mark in the newly polished patch.
Related products
- LOOP-P2 polishing compound - the product this guide uses, with dosage and the three-pass rule.
- LOOP-S1 sealer - reseal the repaired area 24 hours after polishing.