Guide 03 · 24 to 48 hours, mostly waiting
Mixing and using a poultice
A poultice removes a stain by drying out: as water leaves the clay it pulls whatever is dissolved in the stone up into the paste, which you then lift off and throw away. Two mistakes stop that happening, and both of them cost you the full forty-eight hours before you find out.
Choose the liquid first
The clay is inert. What you mix it with decides what will move.
| Stain | Mix with | Dwell | Note |
|---|---|---|---|
| Oil, grease, suncream | A mild solvent | 48 h | Ventilate; the solvent’s own label governs handling |
| Tea, coffee, leaves, wine | 12 % hydrogen peroxide | 24 h | Test on an offcut if the stone is dark or coloured |
| Ink, dye | Peroxide on pale stone, solvent on dark | 24 h | Not acetone on filled travertine - it attacks the filler |
| Unknown but water-soluble | Warm water | 24 h | Always the first thing to try; it cannot make anything worse |
| Rust, iron | - | - | Needs an iron-specific product; peroxide sets iron permanently |
Mixing
Two parts LOOP-R3 powder to one part liquid, by volume. Add the liquid to the powder, not the other way round, and stop while it still looks slightly too dry - clay keeps taking up liquid for a minute after it looks mixed.
The consistency you want holds a soft peak on the trowel and does not run when you hold the trowel vertical. Too wet and it slumps off a wall or a riser; too dry and it will not make contact with the stone across its whole area, which shows up as a blotchy result.
Quantity: 1 kg of powder covers about 0.35 m² at 6 mm. A 20 × 20 cm stain needs a 25 × 25 cm patch of paste once the margin is added, which is 0.0625 m² - about 180 g of powder and 90 ml of liquid. Mix a little more than that; scraping the bowl for the last corner is how patches end up thin.
Applying it
- Clean and dry the area. Dust and loose dirt mix into the paste and get held against the stone for two days.
- Spread 6 mm thick, extending 25 mm beyond the stain on every side. Stains are wider inside the stone than they look on the surface, and a poultice that stops at the visible edge leaves a ring.
- Cover with plastic film and tape three sides only. The open edge is the point: covered completely, the paste never dries and nothing is drawn out; left bare, it dries in two hours and stops working before it has started.
- Wait. Twenty-four hours for organic, forty-eight for oil. Resist looking under the film: lifting it breaks the drying pattern.
- Check that it is dry before removing. It should be crumbly and lighter in colour, and it should come away from the stone cleanly. Still damp means more time, not more force.
- Lift it off dry with a plastic blade, straight into a bag. Removing a wet poultice drags the dissolved stain back into the stone, which is the second of the two mistakes.
- Rinse with clean water, blot, and let the stone dry for 48 hours before you judge the result. Damp stone looks darker and you will think it has failed.
- Assess, and repeat if it has improved. Deep oil often needs two applications, sometimes three. If the third application changes nothing at all, stop - that stain is as out as it is coming.
- Re-seal when the stone is genuinely dry. Four minutes of LOOP-S1, excess wiped. Sealing over trapped moisture leaves a permanent dark patch, which would be a sad end to three days of patience.
- Tape all four sides of the film. This is the single most common reason a poultice does nothing.
- Remove the paste while it is still wet, for the same reason in reverse.
- Let it bake dry in direct sun or over underfloor heating - turn the heating off the day before.
- Wash the leftovers down a drain. Dried clay sets in the trap; bag it as solid waste, as safety explains.
On vertical surfaces
Mix slightly drier, apply in two 3 mm passes rather than one of 6 mm, and tape the film along the top and both sides, leaving the bottom edge open. On a shower wall, turn off the water supply for the duration: one accidental rinse undoes the whole thing.
What a poultice will not do
- Etching. There is nothing inside the stone to draw out; see guide 01.
- Efflorescence. The salt keeps arriving from behind the stone, so you would be drawing out a supply, not a stain.
- Iron from within the stone. If it came with the slab, it stays with the slab.
- A dark patch that is actually trapped moisture. Find and stop the water first; the diagnosis table covers how to tell them apart.
Related products
- LOOP-R3 poultice powder - mix ratios, dwell by stain type and a worked quantity.
- Stain diagnosis - confirm the stain and which liquid to mix before you start.