Guide 02 · one day plus 72 hours of patience

Sealing an unfilled travertine floor

Worked through on a real area - 92 m² of unfilled, honed travertine in an entrance hall. The interesting part is the arithmetic: the right quantity to buy is about 13 litres, and people who read only the headline coverage figure order nine and stop halfway through the second coat.

Before anything, four checks

  1. Moisture. Tape a 300 × 300 mm sheet of clear plastic to the floor on all four sides and leave it overnight. Condensation underneath in the morning means the slab is still giving off water, and sealing now traps it. Wait and test again in a week.
  2. Efflorescence. Any white powder means salts are still migrating. Sealing locks them under the surface, where they will push the sealer off in patches. Dry-brush weekly until a fortnight passes with nothing new.
  3. Age and grout. Give a new floor fourteen days from laying, and grout seven days from grouting. Both are still curing and both will take the sealer unevenly before then.
  4. Temperature. Stone between 8 and 28 °C. Cold stone leaves the sealer sitting on top and drying patchy; hot stone or direct sun dries it before you can wipe the excess off.

How much to buy, worked through

The coverage figure for LOOP-S1 on unfilled travertine is 9–12 m²/L. For ordering, use the low end:

  • First coat: 92 m² ÷ 10 m²/L = 9.2 L
  • Second coat: an absorbent stone takes about 40 % of the first - 3.7 L
  • Total: 12.9 L, so buy 15 L (three 5-litre containers) and keep what is left for the first repair
Why not nine litres

Because 22–26 m²/L is the figure for polished marble, and that is the number that gets quoted. Unfilled travertine drinks about two and a half times as much, and the open pits take more again. Running out mid-floor is worse than over-ordering: the join between a sealed and an unsealed area shows up as a line that needs the whole floor re-done to remove.

The day, in order

Timings for 92 m² with two people. One person should add roughly half again to the application steps.
ClockStepWatch for
Day beforeClean with LOOP-N4 at 1:20, rinse twice, leave to dry overnightAny detergent left behind stops the sealer keying in
08:00Mask skirtings and thresholds; set out the containers and applicatorsSealer on painted skirting dries to a shiny streak
08:30First coat, in 2–3 m² sections, with a microfibre applicatorKeep a wet edge; do not let a section start drying before the next overlaps it
+4 minPer section: wipe off every trace of excess with a dry clothThis is the step that decides whether the floor hazes
11:00Walk the floor with a torch, looking for missed patches and for glossGloss means residue: re-wet that spot and wipe again now
11:15Second coat on the same pattern, 45 minutes after the first was finishedIt should take noticeably less product; if not, the first coat was wiped too hard
14:00Final inspection, masking off, floor closedLight traffic from 6 hours after the last section
+72 hWater, mopping and cleaning allowedMopping at 24 hours is the commonest cause of a floor that «never sealed properly»

If it hazes

A white or cloudy film is sealer that dried on the surface instead of being wiped off. Caught within 24 hours it is easy: wet the area with a little more sealer, agitate it with a white pad or cloth so the dried film redissolves, and wipe it dry immediately. After a day or two it needs a residue remover and a great deal more work, which is why the four-minute wipe is not optional.

Proving it worked

Seven days after sealing, put a few drops of water on the floor in three places and leave them for ten minutes. The stone should not darken. Repeat the same test every six months in the same three places and write the dates somewhere: when the darkening starts coming back, you have your re-sealing interval rather than a guess. On an entrance hall expect eighteen months to two years; on a bathroom floor, three or four.

What this does not do

  • It does not fill the pits. Unfilled travertine still has holes in it, and they will still collect grit.
  • It does not stop etching. Acid attacks the stone itself, not the sealer, and a sealed floor etches as readily as an unsealed one - see guide 01.
  • It does not change the colour. If the floor looks grey and flat and you want it deeper, that is LOOP-C5 instead, not a second coat of this.